The Overmilling Trap: How Laser Diffraction Pinpoints the Milling Endpoint to Cut Energy Costs
2026-11-25News
Key Takeaways
When should you stop wet milling? First, confirm that the product meets its particle size specifications. Then check how much finer the particles get with more milling.
Use laser diffraction to compare D50, D90, and the full particle size distribution at different milling times. In our pesticide suspension concentrate case study, particle size changed very little between 3.5 and 4 h. Compare that trend with measured electricity use to assess the value of stopping sooner.
ANALYTICAL TECHNIQUE
Laser diffraction particle sizing
Why does particle size plateau even as milling continues?
As particles break apart, their total surface area increases. If the formulation cannot keep the finer particles dispersed, they may reagglomerate and offset the gains from further milling.
The isoelectric point (IEP) generally refers to the pH at which a particle’s zeta potential (ζ) or electrophoretic mobility is zero. In suspensions stabilized mainly by electrostatic repulsion, that repulsion weakens near the IEP and particles are more likely to agglomerate. Dispersant adsorption and steric hindrance also affect suspension stability.
When particle size levels off, repeat the measurements and compare results under controlled dispersion conditions. This helps you decide whether to adjust the milling conditions or investigate the dispersion system first.
Case study: What did an extra half hour of milling achieve?
We used the Bettersizer ST to measure the particle size distribution of a pesticide suspension concentrate (SC) at different milling times. The formulation contained an insoluble solid active ingredient dispersed in water.
|
Milling time (h) |
D10 (μm) |
D50 (μm) |
D90 (μm) |
|---|---|---|---|
|
0.5 |
0.365 |
1.015 |
12.39 |
|
1 |
0.363 |
0.982 |
11.25 |
|
2 |
0.375 |
0.893 |
8.623 |
|
3 |
0.354 |
0.886 |
5.772 |
|
3.5 |
0.345 |
0.814 |
4.721 |
|
4 |
0.344 |
0.812 |
4.749 |
Table 1. Particle size percentiles for the pesticide suspension concentrate at different milling times. Data from our application case study on quality testing of pesticide suspension concentrates.
Between 0.5 and 3.5 h, D50 fell from 1.015 μm to 0.814 μm, and D90 fell from 12.39 μm to 4.721 μm. At 4 h, D50 edged down to 0.812 μm, while D90 rose slightly to 4.749 μm. With little further size reduction in the final half hour, around 3.5 h is a candidate milling endpoint to validate for this formulation.
Repeat the measurements to see whether the change in D90 exceeds normal measurement variability. If the slight increase is reproducible, compare dispersion conditions and measure zeta potential to assess whether agglomeration is involved.
If you change the material, formulation, or equipment, measure the particle size trend again against the new targets to identify when to stop milling.
How does laser diffraction help identify the milling endpoint?
Laser diffraction measures the light that particles scatter at different angles and uses an optical model to calculate a volume-based particle size distribution. Comparing size percentiles and distribution curves at different milling times shows which size ranges are changing.
- D50 is the particle diameter below which 50% of the total particle volume falls. It tracks the middle of the distribution.
- D90 is the particle diameter below which 90% of the total particle volume falls. It tracks the coarse end of the distribution.
- The full distribution curve shows the shape of the peaks, the width of the distribution, and the coarse tail.
In this suspension concentrate, D50 fell from 0.893 μm to 0.886 μm between 2 and 3 h, while D90 fell from 8.623 μm to 5.772 μm. Together, the two metrics show that the coarse end was still shifting toward smaller sizes even as the middle of the distribution changed very little.
Use these four steps to set your milling endpoint criteria:
- Define the particle size targets. Set targets for D50, D90, or other distribution metrics based on the product’s intended use. Specify what you need to verify for stability and performance in use.
- Standardize sampling and measurement. Keep the sampling location, dispersion medium, dispersion conditions, and measurement timing consistent so results from different milling times can be compared directly.
- Sample more often as size reduction slows, and repeat the measurements. Compare changes between several consecutive sampling points with measurement variability. Check whether gains remain small and whether the coarse end is still shifting toward smaller sizes.
- Validate when to stop milling. Once particle size meets the specifications and further reduction slows, use product quality checks and measured electricity use to identify the earliest suitable window for stopping.
Verify sample dispersion before assessing the milling process
Before tracking particle size over milling time, verify that the dispersion method gives stable, repeatable results. If agglomerates continue to break apart inside the instrument, successive measurements can show progressively smaller sizes.
In our study on dispersing lithium iron phosphate (LFP) battery material, we used the Bettersizer 2600 with the BT-802 wet dispersion unit to measure the particle size distribution of LFP dry powder dispersed in water. The distribution and obscuration continued to change with longer stirring and circulation. After comparing several ultrasonication conditions for sample preparation before measurement, the study selected 510 W for 1 min for this sample.
Match sample preparation to the measurement objective. To observe agglomeration as it occurs in the milling process, verify that sample preparation preserves that state. To measure particle size after full dispersion, verify that the conditions used to break up agglomerates give stable results.
How do the Bettersizer ST and Bettersizer 2600 support this workflow?
The Bettersizer ST is designed for routine industrial quality control with wet dispersion. It combines wet circulation, ultrasonic dispersion, and particle size measurement. Saved standard operating procedures (SOPs) let you measure D10, D50, D90, and the full distribution under consistent conditions across milling time points.
The Bettersizer 2600 supports wet and dry dispersion configurations and automated SOP-based measurements, helping labs develop dispersion methods for different sample forms. The LFP study used the BT-802 wet dispersion configuration.
How do shorter milling times translate into energy savings?
Verify that the product still meets its specifications after shortening the milling cycle. Then compare measured electricity use per unit of product that meets specifications before and after the change, using the same metering boundaries.
If the mill draws constant input power, estimate electricity savings as follows: electricity saved (kWh) = input power (kW) × time saved (h). Under that assumption, shortening a milling cycle from 4 to 3.5 h reduces electricity use during the milling stage by 12.5%.
Multiply the measured electricity savings by the applicable electricity rate to estimate cost savings. To estimate the associated emissions reduction, use an electricity emissions factor appropriate to the scope of your calculation.
Visit the Bettersize Free Sample Testing page to share your material, dispersion medium, particle size targets, and current process details. Discuss how to track particle size at different milling times with our applications team.
Frequently Asked Questions
What are the warning signs of overmilling in a wet milling process?
Watch for particle size leveling off or the coarse end of the distribution shifting back toward larger sizes. Repeat the measurements to confirm the trend, then check whether the product meets specifications. If it does, use measured electricity consumption to assess the benefit of milling longer.
How do I reset the milling endpoint after changing the formulation?
Measure the particle size trend against the new formulation’s quality requirements. Validate a stopping time within the interval where the product meets specifications and further size reduction slows. The 3.5–4 h interval applies to the pesticide suspension concentrate tested here. You can use the same sampling and analysis approach for your own formulation.
Why track D90 when D50 barely changes?
D90 tracks the coarse end of the distribution and can keep falling even after D50 levels off. Check each metric against your product specifications when deciding when to stop milling.
What should I check if D50 rises after further milling?
Repeat the measurement under the same sampling and measurement conditions. Then compare results under different dispersion conditions. If the increase is reproducible, check pH and zeta potential to assess formulation stability and whether reagglomeration may be occurring.
How can I tell whether particle size changes are related to the isoelectric point?
Measure zeta potential or electrophoretic mobility at different pH values to identify the isoelectric point. Then compare the corresponding laser diffraction particle size distributions to see whether the changes cluster near that pH.
How much can I save on electricity by using particle size analysis to optimize milling?
Cost savings depend on how much less electricity you use and the rate you pay. Verify that the product still meets specifications after the shorter cycle, then compare electricity use and costs per unit of product that meets specifications.
Further Reading
Read the application note on milling pesticide suspension concentrates for the full milling trend plot and particle size data.
|
FURTHER READING / APPLICATION NOTE Want to explore this study further? Read the original application note for the full experimental methods, data, and findings. Read the Original →GCC Powders · Laser Diffraction · Particle Size Distribution |
|
Recent News